running...
How to use
Choose the charge (scrap share, hot-metal silicon), the lime addition, the lance height and the oxygen flow, then press Start heat. The vessel tilts to charge, stands upright for the blow, and the lance drops oxygen onto the bath. Watch carbon fall, temperature climb and the slag form. Stop automatically at the end-point carbon, or press End blow now. Then the steel is sampled and tapped and a verdict compares the result with a typical low-carbon grade. Try an overblow (end carbon 0.02 %) to see FeO and P go the wrong way, or a very low lime charge to see phosphorus stay high.
The science
Oxygen (99.5 % pure, about 3.4 Nm3 per tonne per minute) is blown at supersonic speed onto the bath. It oxidises, in order of affinity, silicon, then mainly carbon, with some iron going to FeO in the slag:
Si + O2 -> SiO2 (0.798 Nm3 O2 per kg Si)
C + 1/2 O2 -> CO (1.866 Nm3 CO per kg C; about 10 % burns on to CO2)
Fe + 1/2 O2 -> FeO (6.41 kg FeO per Nm3 O2)
While carbon is high, its removal is limited by oxygen supply: the carbon rate is a fixed fraction (the blowing efficiency) of the oxygen flow. Below a critical carbon content the rate is limited by carbon transport to the reaction zone and falls roughly linearly with C, which gives the exponential tail seen on the chart. Surplus oxygen goes to FeO, so overblowing wastes iron and oxidises the slag. A higher lance (soft blow) puts more oxygen into the slag and less into carbon.
dC/dt = -k C, C < C_crit (efficiency = eta0 * C/C_crit)
The energy balance is what makes the process autothermal. Oxidation of Si, C and Fe releases heat; melting the scrap, heating the lime and ordinary losses take it away: dT = (Q_oxidation - Q_scrap - Q_lime - Q_loss) / (m * cp) with cp = 0.84 kJ/kg/K. More scrap cools the bath (a coolant), more silicon heats it. Phosphorus leaves into a basic (CaO/SiO2 above about 3), oxidising, cooler slag; the model uses an empirical partition ratio that grows with basicity and FeO and falls with temperature.
Simplifications. One lumped metal bath and one slag, no gas-metal-slag emulsion, no manganese, sulphur or nitrogen, constant post-combustion share, empirical dephosphorisation constants that are not calibrated to a real plant, no splashing or slopping, no off-gas dust. The vessel is drawn with a cut-away; sizes are schematic. Values are illustrative, and typical of a 100 t BOF, not a plant guide.