loading...
running...
The science
What the model solves. One electrolytic cell of a copper tankhouse (default 36 anodes, 37 cathodes, 360 kg anodes) with its electrolyte, followed by the plant that treats the anode slime. Every step it updates (1) the cell current, voltage and copper mass balance from Faraday's law, (2) the composition and amount of anode slime released as the anodes dissolve, (3) the copper, nickel and silver in the electrolyte, and (4) the flowsheet that turns the slime into selenium, tellurium and dore bullion. The 2D and 3D pages run the same code and show identical numbers.
Faraday's law. Dissolving or depositing one mole of Cu needs two moles of electrons, so one ampere-hour moves M / (zF) x 3600 = 1.1855 g of copper:
mdep = η I t M / (z F), mdiss = (1 + χ) I t M / (z F), z = 2, M = 63.546 g/mol, F = 96485 C/mol
The cathode gets only the current efficiency η (short circuits and stray current lose the rest, slider); the anode dissolves a little more than Faraday predicts because oxygen and acid also attack copper chemically (χ, slider). The surplus Cu2+ would raise the electrolyte concentration without limit, so a bleed stream sends part of the electrolyte to purification. The check "Copper balance" verifies dissolved = electrolyte gain + cathode + bleed + entrained in slime to rounding error.
Cell voltage and energy. The voltage is a sum of resistive and kinetic terms:
V = ηov(j) + j (g / κ + d / (κ ε1.5)) + I Rbus
with g the anode-cathode gap, κ the electrolyte conductivity (an empirical function of temperature, acid, Cu and Ni content, about 62 S/m at 65 C), d the thickness of the clinging slime layer, ε = 0.55 its porosity (Bruggeman exponent 1.5) and Rbus the contact and busbar resistance. ηov = 0.08 + 0.02 ln(j / 250) V lumps the anodic and cathodic overpotentials; it is a fit, not a derived value. The energy per tonne of cathode copper follows from Faraday's law: E = 843.5 V / η kWh per tonne (843.5 kAh moves one tonne of copper at 100 % efficiency), about 270 kWh/t with the defaults. A thick slime layer and a cold, weak electrolyte both raise V; high current density raises copper output per cell but also volts per tonne.
Where the slime comes from. Impurities that are more noble than copper (Ag, Au, Pd, Pt) or that form insoluble compounds (Se and Te as Cu2Se, Ag2Se, Cu2Te, lead as PbSO4, Sb/As/Bi oxides) do not dissolve and fall away as a sludge, while nickel dissolves and builds up in the electrolyte. For every kilogram of anode metal that goes away, element i is released as xi kg and retained in the slime with a fraction ri (Au 0.999, PGM 0.99, Pb 0.97, Se 0.95, Te 0.92, gangue 0.4). Silver is special: a small share dissolves as Ag+, and chloride precipitates it as AgCl, so rAg = 0.90 + 0.099 (1 - e-Cl/15). With no chloride about 10 % of the silver stays dissolved and some co-deposits on the cathode (the page estimates it assuming half does). Copper bound as Cu2Se / Cu2Te (2 MCu / MSe = 1.61 kg Cu per kg Se) is part of the slime, and a slider sets the share of entrained copper (fines and salts). A share of the slime clings to the anode and forms the resistive layer; the rest falls to the sump, which is cleaned at every anode change. Typical real slime is a few kg per tonne of anode.
Treatment flowsheet. The slime stock of the last anode cycles is processed by the usual chain:
Cu + H2SO4 + ½ O2 → CuSO4 + H2O (decopperising leach: 1.543 kg acid and 0.252 kg O2 per kg Cu)
Cu2Se + Na2CO3 + 2 O2 → Na2SeO3 + 2 CuO + CO2; H2SeO3 + 2 SO2 + H2O → Se + 2 H2SO4 (1.62 kg SO2 per kg Se)
Te + 2 Cu → Cu2Te (cementation with copper powder, 0.996 kg Cu per kg Te at 1.0 x stoichiometric)
2 Ag+ + Cu → 2 Ag + Cu2+ (cementation: 3.39 kg Ag per kg Cu; excess Cu stays in the cement as an impurity)
What is left after the leach and the Se and Te steps (silver, gold, PGMs and a little of everything else) is smelted to dore bullion, whose silver and gold are then separated by a Moebius electrolytic cell or by parting plus cementation. The recoveries of every step are sliders. The "Flowsheet silver closure" check verifies that the silver fed equals the silver in cement, Moebius cell and slag, and the cementation check compares the copper consumed with (nAg/2) MCu.
Honest simplifications. The cell is lumped: one current density, one electrolyte concentration, no gradients, no cathode nodulation, no passivation, no electrolyte temperature balance. Slime composition, retention fractions and the conductivity law are typical textbook-size values, not data for a particular plant. Selenium speciation is fixed at 60 % Cu2Se, 40 % Ag2Se. The flowsheet is the classic route; modern plants use pressure leaching, chlorination or other chemistry, and the page does not model reaction rates or reagent costs. Plates are drawn at 1.5 times the real pitch so they stay visible. This is an educational model of a safe, inanimate industrial process; it is not an operating guide.